Hongqiang Mould logoHongqiang Mould

Two of Five Moulding Resins Break Down Without a Dryer (6 Processing Guides Checked)

Two of Five Moulding Resins Break Down Without a Dryer (6 Processing Guides Checked)

← Back to Blog · Two of Five Moulding Resins Break Down Without a Dryer (6 Processing Guides Checked)

Drying rules are resin-specific, not shop-wide. PC needs 120 °C for 2–3 h to hold 0.02% moisture; PA66 needs 4 h at 80 °C; ABS needs 2–4 h at 80 °C; PP and PE normally need nothing but dry storage. We help moulders and importers turn a resin grade into a complete processing plan, and this article shows where the plan starts.

Every RFQ names a resin. Very few name a moisture limit. The two lines are not the same thing, and the gap between them decides how the first trial runs.

One camp dries every pellet out of habit. The other switches the dryer on only for nylon. Both camps can point to good parts, and both can point to scrapped ones.

The difference is rarely effort. It is whether the drying spec matched the resin in the hopper. We set out to answer four questions:

  • Which of PP, PE, ABS, PC and PA actually absorb moisture into the pellet?
  • What temperature, time and moisture ceiling does each published data sheet set?
  • What must the drying air deliver besides heat, and where are the exceptions?
  • What should an RFQ state so drying is planned, not improvised?

Across six manufacturer and compounder guides, one pattern holds: two of the five resin families degrade chemically without a dryer, one complains on the surface, and two mostly need dry storage.

The six documents agree on the split. Covestro holds Makrolon 2558 to 120 °C, 2–3 h and a 0.02% ceiling. BASF dries Ultramid A4H for 4 h at 80 °C into a 0.03–0.06% window. INEOS Styrolution dries Terluran for 2–4 h at 80 °C under 0.1%. Asahi Kasei and The Plastics Group keep neat PP and PE off the dryer unless surface moisture appears. Wittmann rates Drymax process air down to a −60 °C dew point. A shop that runs all five families carries two drying disciplines at once, and the RFQ should say which one applies.

Key takeaways

  • Two families degrade, two coast, one sits between: PC and PA66 need a dryer to hold 0.02–0.06% moisture; PP and PE are not hygroscopic; ABS splits the difference at 0.1%.
  • PC runs hotter, PA runs longer: Covestro sets Makrolon 2558 at 120 °C for 2–3 h; BASF sets Ultramid A4H at 80 °C for 4 h.
  • ABS forgives at 0.1%: INEOS Styrolution calls 2–4 h at 80 °C usually sufficient, and a vented screw can replace the dryer on dry-stored pellets.
  • Surface moisture is the only PP risk: up to 0.2% moisture leaves properties untouched per Asahi Kasei; appearance parts are the exception.
  • The dryer has its own spec: desiccant units reach a −60 °C dew point (Wittmann Drymax); hot-air hoppers only handle surface moisture.

Methodology

This comparison reads published specs, not new lab runs. We collected the drying sections of six primary documents: the Covestro Makrolon 2558 product page, the BASF Ultramid A4H product information, the INEOS Styrolution Terluran shop page with its technical data sheet, the Asahi Kasei polypropylene processing guide, a TPO processing guide from The Plastics Group of America, and the Wittmann dryer range page.

Every drying value quoted below is a manufacturer recommendation for one named grade or resin family. Shop facts on our side cover a different thing: PP, PE, ABS, PC and PA are the five families we mould on 11 presses spanning 80 to 450 T, with design, machining, trials and bridge CMM inspection in one plant. We did not instrument drying air for this article, so anything beyond the published numbers is marked as industry-typical.

Where a claim needs a mechanism rather than a spec, we say so and keep it short. The Limitations section below carries the boundaries.

Why does water in a pellet change the part at all?

Water reaches the melt by two routes. Hygroscopic resins pull moisture inside the pellet during storage; non-hygroscopic resins only carry it on the surface. Both routes end as steam at melt temperature.

The absorbed kind does more damage. In polymer chemistry terms, moisture at melt temperature breaks polymer chains in condensation-prone resins, so producers answer with a moisture ceiling: 0.02% for PC per Covestro, 0.03–0.06% for PA66 per BASF. The Terluran data sheet puts ABS saturation at 1.03% water and the working equilibrium at 0.21%, which is why INEOS asks processors to predry below 0.1%.

Surface moisture, the route PP and PE take, mostly shows up as appearance faults such as splay streaks and gloss marks, rather than lost strength, per the Asahi Kasei guide. The boundary has a cost side too: condensation forms on pellets moved from cold storage into a warm hall, and The Plastics Group tells moulders to let sealed containers equalise for 24 hours before opening.

Mould plate with six sliders and lifters prepared for an undercut housing program
A fitted mould plate waits for trial. The resin grade it will run decides the drying step before the first shot.

What does each resin data sheet ask for?

Five families, five rows. Read the temperature column first, then the ceiling.

Resin (named grade)Drying temperatureDrying timeMoisture ceilingPublished source
PC — Makrolon 2558120 °C2–3 h≤ 0.02%Covestro product page
PA66 — Ultramid A4H80 °C4 h0.03–0.06%BASF product information
ABS — Terluran GP-2280 °C2–4 hbelow 0.1%INEOS Styrolution shop page
PP — neat resinusually none; 75 °C if needed2 hsurface moisture onlyAsahi Kasei processing guide
PE / TPOusually none; 82–99 °C if needed1–2 h; 24 h maximumsurface moisture onlyTPO processing guide

PA dries low and slow. PC dries hot and short. Absorbed water, not machine power, sets both schedules.

Specs are grade-level facts. Makrolon 2558 does not speak for every PC on the market, so confirm the grade before quoting a ceiling to your customer.

What should the drying setup deliver besides heat?

Temperature alone under-dries hygroscopic pellets. The air must carry the moisture away, and the dryer type decides how far that works. Desiccant dryers strip moisture from the process air itself; Wittmann rates the Drymax range down to a −60 °C dew point. Hot-air hoppers only warm ambient air, which moves surface moisture and little else.

ItemValue and condition
Dew point, desiccant dryerdown to −60 °C (Wittmann Drymax range spec)
Hot-air hopper rolesurface moisture only; suits PP and PE
Vented-screw exceptionABS predrying can be skipped when pellets stayed dry (INEOS)
Regrind handlingabsorbs moisture faster than virgin pellets; dry before reuse (INEOS)
Over-drying guardPA66 viscosity climbs past spec (BASF); TPO cap 24 h (TPG); Wittmann MPF lowers temperature at stoppage

Check the exception column before buying steel. A vented screw or a sealed conveying line can remove a drying step entirely.

How does this change an RFQ?

  • Name the grade, not the family. Makrolon 2558 and a generic PC answer to different ceilings.
  • Put the moisture number on the drawing or purchase note, next to the dimensions it protects.
  • Ask which dryer type feeds the press. Desiccant and hot-air units are not interchangeable for PA.
  • Declare regrind share in advance; INEOS reports it absorbs moisture faster than virgin pellets.
  • Ask how conformity gets checked. Moulded parts here pass the bridge CMM room before approval.

None of these lines cost money at quotation stage. All of them move defects out of the first trial.

Bench-top force tester checking a moulded sample at the inspection bench
Moulded samples checked at the inspection bench before a report goes out.

Limitations

Data sheets describe one resin and one dryer in isolation. Hopper load, ambient humidity and stoppages move real outcomes. BASF says it directly: drying time depends on initial moisture, temperature and the dew point of the drying air.

Every number above comes from a manufacturer or compounder document, checked on 28 October 2026. We ran no drying tests ourselves. The values are recommendations, not warranties, and each grade needs its own data sheet before production.

What this means for your RFQ

Moisture is the cheapest variable on a moulding program and the easiest one to leave unstated. A moisture limit written beside the dimension travels with the part; a drying habit stays behind in the workshop.

Send your drawing and resin name to info@hongqiangmould.com or WhatsApp +86 199 6437 6528. The quote lands within 24 hours, with the drying spec, tooling plan and bridge CMM checks attached to it.

Specified | Dried | Verified.

Frequently asked questions

Which injection moulding resins need drying before moulding? PC and PA66 need a desiccant dryer before moulding; ABS needs one in most cases; PP and PE normally do not. Covestro caps PC moisture at 0.02 percent, BASF dries PA66 for 4 hours at 80 °C, and INEOS Styrolution asks for under 0.1 percent on ABS. PP and PE mainly carry surface moisture, which dry storage prevents.

What happens if you mould wet polycarbonate or nylon? Melted resin turns trapped water into steam, and steam marks the part as splay, bubbles or brittle fracture. That is why the PC ceiling sits at 0.02 percent. Over-drying has its own cost: BASF notes that PA66 melt viscosity climbs when granules are dried past the recommended window.

How long should ABS be dried at 80 °C? Two to four hours at 80 °C, per the INEOS Styrolution data for Terluran. The residual moisture target stays below 0.1 percent. Circulating dryers can need longer, regrind absorbs moisture faster than virgin pellets, and a vented screw can replace predrying when the pellets were stored dry.

Does polypropylene need a dryer before injection moulding? Usually not. Asahi Kasei states that up to 0.2 percent moisture does not change the physical properties of polypropylene, so drying is not typically required. Surface moisture from cold storage or high humidity can still mark appearance parts. When drying is needed, the guide sets 2 hours at 75 °C in a desiccant dryer.

Jack works on the tooling and molding team at Hongqiang Mould, an injection mould manufacturer and plastic injection molding supplier. The shop runs 11 presses from 80 to 450 T, 5 CNC machining centres and a metrology room with bridge CMM inspection.


Technical Guides

Browse all technical guides →