We help buyers size a cavity against the resin before any steel is cut, not after the first sample measures small. The cavity dimension is the part dimension divided by (1 − shrink), never the part multiplied by (1 + shrink). At 2.5 % shrink that single operation costs 0.19 mm on a 300 mm part.
A finished part is measured. The cavity that made it is not. When a first sample comes back four tenths under the drawing, the instinct is to blame drift in the tool. Often nothing drifted. The cavity was cut to a figure that came out of the wrong operation, and that figure now sits in hardened steel by design.
Two habits sit on either side of the problem. In the first, the drawing asks for a cavity at nominal size and the moulder is expected to absorb shrink somewhere downstream. In the second, the toolmaker takes the part dimension and adds the datasheet shrink rate: part 100 mm, resin shrinks 2 %, so the cavity is cut at 102 mm. The first habit leaves the decision unowned. The second picks the right direction and the wrong arithmetic.
The contradiction is where the definition points. Shrinkage is measured against the cavity, not against the part. ASTM D955-21 writes it as the cavity dimension minus the part dimension, divided by the cavity dimension. Turn that definition around to solve for the cavity and the operation becomes a division. Almost everyone reaches for a multiplication instead. The two agree closely at small values and pull apart as the resin shrinks more.
Four questions frame what follows:
- What fixes the shrinkage figure, and why does the definition decide the operation?
- How much does each common resin shrink, and how far apart are the flow and cross-flow numbers?
- How large is the gap between dividing by (1 − S) and multiplying by (1 + S), and when does it matter on a real drawing?
- What should an enquiry carry so the cavity is sized once and not re-cut?
Short answer, assembled from two published standards and one resin supplier data sheet. The cavity is the part divided by (1 − shrink). The gap between that and the multiplier shortcut grows with the square of the shrink rate, so it is invisible on a small PC part at 0.6 % and decisive on a long HDPE part at 2.5 %. A filled grade then needs two figures rather than one, because the same resin can shrink 0.53 % along flow and 1.02 % across it.
Key takeaways
- Division, not a multiplier: the cavity is the part divided by (1 − shrink), so a 100 mm part in a 2 % resin takes a 102.04 mm cavity against 102.00 mm from the shortcut.
- The gap follows the square: the error is the part dimension times the shrink rate squared, which is 0.02 mm at 2 % on a 60 mm part and 0.19 mm at 2.5 % on a 300 mm part.
- One resin, two shrink rates: BASF reports its PA66-GF30 grade at 0.53 % along flow and 1.02 % across it under ISO 294-4, and one cavity figure cannot honour both.
- Unfilled grades spread eightfold: ABS sits at 0.4–0.7 % and HDPE at 1.5–3.5 %, so the resin choice moves cavity oversize more than any tooling decision does.
- The definition sets the denominator: ASTM D955-21 measures shrink against the cavity, and that is why the correction divides rather than adds.
- Glass cuts shrink by half to two-thirds: SABIC puts reinforced compounds at one-third to one-half the shrink of the neat resin, so a 1.5 % unfilled grade lands near 0.5–0.75 % once it is filled.
Methodology
The numbers below come from published documents rather than from a shrink study run on our floor. ASTM D955-21 supplies the definition and the 24-hour and 48-hour measurement points. ISO 294-4:2018 supplies the two-direction measurement method that filled grades depend on. The single grade-level figures come from BASF product information for Ultramid A3EG6, a 30 % glass-fibre PA66, which reports its own shrink under both methods. The resin ranges in the first table come from two independent compilations built out of supplier processing datasheets, not from one trial. Any cavity dimension shown here was calculated from a published shrink rate, and the arithmetic is left visible so it can be re-run on a different part.
What fixes the shrinkage figure, and why does the definition decide the operation?
Shrinkage is the difference between the cavity that formed the part and the part itself, expressed against the cavity. ASTM D955-21 states it that way, and ISO 294-4:2018 works from the same basis. Read the definition literally and the arithmetic is settled before any number is chosen: the cavity is the denominator, so solving for the cavity is a division.
Written out, the ratio is S = (C − D) / C, where C is the cavity dimension and D is the part dimension one day or two days after moulding. Rearranged for the cavity, that becomes C = D / (1 − S). The shortcut most people use instead is C = D × (1 + S). Both expressions move in the same direction, and both grow as the shrink rate grows. They simply do not land on the same number.
The standard is honest about what its own figure can carry. ASTM D955-21 notes that testing on a standard specimen gives comparable data between materials, and cannot predict the absolute size of a real part. Flow path, wall thickness, packing pressure and mould temperature all move the result. The datasheet rate is therefore a starting value, and the operation applied to it is what determines whether the starting value lands close or far.
How much does each common resin shrink, and in which direction?
The spread between grades is wider than most drawings assume. The table below collects ranges from two independent compilations of supplier data. Every figure below is industry-typical, and we did not measure any of it ourselves.
| Resin | Shrinkage range (industry-typical) | Behaviour and direction note |
|---|---|---|
| ABS | 0.4–0.7 % | Amorphous; nearly equal flow and cross-flow |
| PC | 0.5–0.8 % | Amorphous; nearly equal flow and cross-flow |
| PA66, unfilled | 0.8–1.5 % | Semicrystalline; direction widens with fill level |
| PP homopolymer | 1.0–2.5 % | Semicrystalline; copolymer grades run higher |
| HDPE | 1.5–3.5 % | Widest range of the unfilled commodity grades |
| POM | 1.8–2.5 % | Semicrystalline; slow crystallisation, late shrink |
| PA66-GF30, along flow | 0.53 % | BASF A3EG6, ISO 294-4 parallel direction |
| PA66-GF30, across flow | 1.02 % | BASF A3EG6, ISO 294-4 normal direction |
Read the last two rows together. One grade, one test method, two figures that differ by roughly double.
Two things follow. The first is that the resin choice is the largest single lever on cavity oversize: moving from ABS to HDPE multiplies the correction by roughly five. The second is that a filled grade cannot be sized from a single number, because the fibres align with flow and hold the part closer along that axis. SABIC puts reinforced compounds at one-third to one-half the shrink of the neat resin, which is consistent with the BASF figures against unfilled PA66 at 0.8–1.5 %. But this does not cover everything, since fibre orientation shifts with gate position and wall thickness, so the two datasheet directions mark the ends and not the whole field.

How large is the gap between dividing and multiplying?
The gap is small until it is not. Subtract the shortcut from the correct expression and the difference reduces to D × S² / (1 − S), which is a shade under the part dimension times the shrink rate squared. That is why the error stays hidden on short parts in low-shrink resin and shows up on long parts in high-shrink resin. The table below runs six part and resin combinations through both operations.
| Part | Shrink rate | Cavity by division, D / (1 − S) | Cavity by multiplier, D × (1 + S) | Gap |
|---|---|---|---|---|
| 60.00 mm | 2.0 % | 61.22 mm | 61.20 mm | 0.02 mm |
| 100.00 mm | 0.53 % | 100.53 mm | 100.53 mm | 0.00 mm |
| 120.00 mm | 0.5 % | 120.60 mm | 120.60 mm | 0.00 mm |
| 150.00 mm | 1.8 % | 152.75 mm | 152.70 mm | 0.05 mm |
| 200.00 mm | 2.5 % | 205.13 mm | 205.00 mm | 0.13 mm |
| 300.00 mm | 2.5 % | 307.69 mm | 307.50 mm | 0.19 mm |
Scan the last column, not the first. The error is negligible on the glass-filled part and real on the long HDPE one.
Two patterns sit in that column. The error climbs with the shrink rate rather than staying fixed, so a 2.5 % resin is not simply twice as bad as a 1.25 % one. And it climbs with part length on top of that, so a long part in a high-shrink resin is where the shortcut finally fails. On a 300 mm HDPE cover, 0.19 mm is often the difference between a part that passes and a part that is scrapped on a tight drawing. This does not mean every cavity needs the division. It means the operation should be chosen by the tolerance on the drawing rather than by habit.
What should an enquiry carry so the cavity is sized once?
The cavity is cut to a number agreed at quotation, and it is expensive to revisit once inserts are hardened. Most of the cost of a re-cut is not the machining. It is the weeks lost while the tool is out of the press. The list below is the set of inputs that let the correction be made once, in the right direction, before the first cut.
| Field | Value to put on the drawing |
|---|---|
| Cavity basis | Part dimension ÷ (1 − shrink), not part dimension × (1 + shrink) |
| Shrink source | Per-grade datasheet value, measured to ISO 294-4 or ASTM D955 |
| Direction | Flow and cross-flow quoted separately for any filled grade |
| Wall basis | One shrink figure per nominal wall; flag any wall that departs from it |
| Tolerance class | Named per ISO 20457 or DIN 16742, not left as a general note |
| Critical dimensions | The two or three sizes that must hold, marked on the drawing |
| Gate position | Agreed before design, because flow direction follows the gate |
Name the gate position, because flow direction follows it and the two shrink figures follow flow.
Two of those fields do most of the work. The shrink source decides whether the starting value reflects the exact grade or a generic family figure, and the direction note decides whether a single number is asked to cover two. Where a buyer leaves both blank, the cavity gets sized on an assumption, and the assumption is usually the multiplier. In our shop the design desk, the CNC and EDM sections, the surface grinder and the CMM room sit in one building, so a cavity dimension is set, cut, trialled and measured without leaving the floor. That is where a division checked at first article stays inside tool tuning rather than becoming a rebuild.

Limitations
Every shrink figure here is a standard specimen value and not a measurement of a real part. ASTM D955-21 says as much about its own test: a plaque gives comparable data between materials and cannot predict the absolute size of a production component. A wall that varies in thickness, a long flow path or a hot spot near the gate all move the result away from the datasheet number, and the trial is what settles it.
The ranges in the first table come from third-party compilations rather than from us. Two were used and they agree on the ordering but not always on the endpoints, so a range is shown where a single figure would be false precision. We do not publish a shrink rate for any resin, because we have not measured one. The grade-level numbers belong to BASF and are quoted as its product information, and the reinforcement ratio belongs to SABIC. Where a document gives a range, this page repeats the range instead of picking a midpoint.
Documents drawn on: ASTM D955-21, Standard Test Method for Linear Dimensional Changes of Plastics, astm.org/d0955-21.html; ISO 294-4:2018, Plastics — Injection moulding of test specimens — Part 4, iso.org/standard/75231.html; BASF product information for Ultramid A3EG6, download.basf.com; SABIC LNP compounds processing guide, sabic.com/en/products/documents/lnp-konduit-compounds-portfolio-introduction/en; and two resin shrinkage compilations, plastikcity.co.uk/useful-stuff/material-shrinkage-rates and plasticxperts.com. ISO 20457:2018 and DIN 16742 are named as tolerance systems, not quoted for specific grades.
What this means for your RFQ
The cavity dimension is fixed while the tool is still a drawing, and that is the cheapest place to fix it. The correction is one division, and it needs two inputs that belong in the enquiry: the exact resin grade, and whether the part carries fibre. Send a 2D or 3D file with the wall basis and the critical dimensions marked, and the cavity can be sized before any steel is cut. Leaving the grade or the direction out is what sends a tool back for a re-cut, the same way that three missing RFQ inputs restart a lead time. From a small PC bracket at half a percent to a long HDPE panel at two and a half, the operation is the same one.
Send the drawing and the resin grade to sales@hongqiangmould.com. A quote is back inside 24 hours. Sized | Cut | Measured
Frequently asked questions
How do you size a mould cavity for shrinkage? Divide the part dimension by one minus the shrink rate. A 100 mm part in a resin that shrinks 2 percent needs a cavity of 100 divided by 0.98, which is 102.04 mm. Multiplying the part by 1.02 gives 102.00 mm, and the difference grows with the shrink rate.
How much does the shrink rate change the final part size? The gap between the two methods is the part dimension times the shrink rate squared. At 2 percent on a 60 mm part it is 0.02 mm, which sits below most tolerances. At 2.5 percent on a 300 mm HDPE part it reaches 0.19 mm, which fails a tight drawing.
Which resins shrink the most and the least? Unfilled HDPE leads at roughly 1.5 to 3.5 percent, and unfilled POM and PP follow at 1.0 to 2.5 percent. Amorphous grades sit lowest, with ABS at 0.4 to 0.7 percent and PC at 0.5 to 0.8 percent. These are industry-typical ranges rather than measurements of one grade.
Why does a glass-filled part need two shrink figures? Glass fibres align with the melt flow, so the part shrinks less along that direction than across it. BASF reports its PA66-GF30 grade at 0.53 percent along flow and 1.02 percent across it under ISO 294-4. One cavity cannot be sized to both with a single number.
Can a cavity be corrected after the first sample? Yes, and a small correction is routine. Weld and re-machine can move a dimension by a few tenths of a millimetre, and hardened inserts can be re-cut or replaced. Sizing the cavity by division first keeps most corrections inside tool tuning rather than a rebuild.
Jack works on the tooling and molding team at Hongqiang Mould, an injection mould manufacturer and plastic injection molding supplier. The shop runs 11 presses from 80 to 450 T, 5 CNC machining centres and a metrology room with bridge CMM inspection.