A cosmetic gate mark costs less than a short-packed part, yet most drawings treat the opposite as obvious. Resin supplier guides place the gate depth floor between 45% and 80% of the wall thickness, and glass-filled grades sit at the top of that band. Cut below the floor to hide the vestige and the packing window closes early, right where the section is thickest. This article compares the published bands from five guides and lists the four inputs that decide the gate before steel is cut.
Most RFQs that reach our desk describe the cosmetic faces in detail and say nothing about the gate. The gate type appears somewhere in the notes, usually as “appropriate gate”, with no depth, no land and no face called out.
Two instincts collide on that silence. One camp treats the gate mark as a defect to hide at any cost, so the gate gets smaller and smaller. The other camp treats the gate as the packing throttle, a feature no drawing line should shrink.
The contradiction shows up on the same part. Buyers who demand an invisible vestige often reject the sink marks and voids that an undersized gate leaves in the thick section, without connecting the two outcomes.
This comparison pulls four questions out of those exchanges:
- Why does published gate depth stop at a floor, not at an aesthetic judgement?
- Where should the vestige land so the mark never matters?
- Where do five supplier guides disagree about the same feature?
- What changes when the resin carries glass fibre?
The short version: Eastman suggests a gate at 50%–80% of the wall for its copolyesters, the DuPont Zytel HTN and Crastin guides want at least 50% of the wall unfilled and up to 75% filled, the RYNITE PET guide caps the band at 75%, and the Minlon/Zytel moulding manual works from 45% to 75%. Five guides, one feature, four different bands — and every one of them ends well above the depth a hidden mark would suggest.
Key takeaways
- Depth floor: half of the wall thickness is the published minimum — Eastman bands 50%–80% of wall, the DuPont nylon manual starts at 45%
- Reinforced premium: glass-filled grades move to the top of the band, up to 75% of wall, to limit fibre breakage and shear
- Blush floor: Eastman warns against gate thickness below 1.65 mm on its copolyesters — smaller gates shear more, and the blush shows next to the mark
- Tunnel limits: Eastman sets the entry angle at 45°–60° with a land of 1.5 mm maximum; DuPont draws 25°±5° and a land of 1 mm for its nylons
- Type decides the mark: submarine, pinpoint and valve gates place the vestige on non-cosmetic faces — the depth does not have to shrink for the mark to disappear
- Direction of correction: gates enlarge with a grinder at trial; shrinking a gate needs welding and re-machining, so start steel-safe at the small end
Methodology
Every number in this article comes from published resin supplier guidance, not from our own trial logs. We read five guides in full: the Eastman Processing and Mold Design Guidelines, the DuPont molding guides for Zytel HTN, Crastin PBT and RYNITE PET, and the DuPont moulding manual for Minlon and Zytel resins. Each value was copied with its context — which resin family, which gate style, which limitation the supplier attached.
The classification of vestige behaviour (which gate type degates automatically, where each mark lands) was cross-checked against industry media coverage, because the resin guides discuss vestige only as a selection input. Shop facts come from our own plant records: five CNC machining centres, EDM and grinding under the same roof as the mould shop, and eleven injection presses covering 80 T to 450 T of clamping force. No gate depth was measured on a press for this article, and none of the published values is presented as our own result.
Why does gate depth stop at a floor?
The gate is the last section to freeze, so its thickness controls how long holding pressure keeps feeding the cavity. The Crastin guide states the logic directly: a minimum gate thickness of 50% of the wall exists “in order to allow for proper packing”. The Minlon manual adds the failure mode: gates that are too small usually increase shrinkage and warpage, and raise the risk of fibre breakage on filled grades.
A smaller gate does hide the mark. It also freezes earlier, and the packing window dies with it — the same window the part weight plateau method measures on a press.
| Guide | Resin family | Gate depth guidance | Land guidance |
|---|---|---|---|
| Eastman Processing and Mold Design Guidelines | Copolyesters | 50%–80% of wall; avoid below 1.65 mm | Edge gate 1.0–1.5 mm |
| DuPont Zytel HTN Molding Guide | PA66, HTN | ≥50% of wall unfilled; up to 75% reinforced | Pin gate a ≥ 0.5 T unfilled, ≥ 0.75 T reinforced |
| DuPont Crastin PBT Molding Guide | PBT | ≥50% of wall unfilled; up to 75% reinforced | Tunnel gate 0.5–0.75 T |
| DuPont RYNITE PET Molding Guide | PET | 50%–75% of part thickness | Edge gate 0.5–1.0 T, land ≤1 mm |
| DuPont Minlon/Zytel Moulding Manual | PA66, Minlon | 45%–75%; rectangular gate 65% | Land ≤1 mm; tunnel Ø 0.7–2.5 mm |
Read the floor first, then the ceiling. Every guide ends its band well above a depth that would hide a mark on a visible face.

Where should the vestige land?
The mark is a geometry problem, and geometry has better answers than shrinkage. Submarine gates tunnel below the parting line and shear the vestige onto a hidden face as the part ejects. Pinpoint gates on a three-plate mould leave a small scar on the non-cosmetic side. Valve gates close over a controlled pin and leave the smallest witness of all, which is why the Crastin guide bans direct gating on aesthetic parts while pointing hot-runner systems at exactly this problem.
Edge, tab and sprue gates remain legitimate choices. They just require a face that the drawing has declared acceptable, and a trim plan for the removal.
| Gate type | Where the mark lands | Degating | Watch-outs |
|---|---|---|---|
| Edge gate | Parting-line edge, on the declared face | Manual or robotic trim | Visible scar; simplest to machine and enlarge |
| Tab gate | Sacrificial tab at the edge | Manual trim of tab | Extra removal step; protects the surface from shear |
| Submarine (tunnel) gate | Hidden face below the parting line | Automatic at ejection | Shear on sensitive resins; geometry limits size |
| Pinpoint gate | Non-cosmetic face, three-plate mould | Automatic at ejection | Small vestige; watch flow balance in multi-cavity tools |
| Valve gate | Controlled entry, often on a hidden floor | Automatic, pin-controlled | Highest tooling cost; smallest witness mark |
| Sprue (direct) gate | Centre of the visible face | Manual removal | Largest vestige; strong packing for single-cavity tools |
Hide the mark by moving it, not by thinning it. The two rows that degate automatically keep both the appearance and the packing window.
Where do five guides disagree on one feature?
The disagreement is the information gain here, because most articles quote a single number as if it were law. On tunnel gates, Eastman draws an entry angle of 45°–60°, a maximum tunnel length of 50 mm, a land of 1.5 mm and a 5°–20° taper for ejection. The DuPont nylon manual draws 25°±5° on its tunnel sections, keeps the land at 1 mm or less, and allows tunnel diameters from 0.7 mm up to 2.5 mm.
Neither guide is wrong. Each band was written for its own resin family, its own viscosity range and its own gate-breaking behaviour at ejection.
| Parameter | Eastman (copolyesters) | DuPont nylon manual (PA66, Minlon) |
|---|---|---|
| Tunnel entry angle | 45°–60° | 25°±5° |
| Gate land | ≤1.5 mm (tunnel); 1.0–1.5 mm (edge) | ≤1 mm |
| Tunnel diameter range | Not stated as a band | 0.7 mm minimum to 2.5 mm maximum |
| Tunnel length / taper | ≤50 mm; taper 5°–20° | Long-tunnel design flagged as critical |
| Gate thickness band | 50%–80% of wall | 45%–75% of part thickness |
Copy the band that matches your resin, not the one that reads best. When the drawing names a different supplier, ask for that guide before the steel is ordered.
What changes when the resin carries glass?
Three things move at once, and all of them push the gate bigger. First, the depth band rises: the Crastin and Zytel HTN guides recommend up to 75% of the wall for reinforced grades, against 50% unfilled, to limit fibre breakage and the higher shear that comes with viscosity. Second, the small point gates gain conditions: the nylon manual allows tunnel and pin gates on glass-filled nylon only above a 0.7 mm diameter. Third, some gate styles drop out entirely — banana gates are “not generally recommended” for the filled and unreinforced engineering grades alike in the DuPont guides.
Uniform fibre orientation is part of the same logic. Guides prefer gate styles that deliver a uniform filling pattern for filled materials, because point-type gates leave the fibres broken and the orientation scattered around the entry.
Limitations
Published bands are guidance, not press measurements. Resin temperature, injection speed and wall geometry shift the real floor on a specific part, which is why toolmakers cut gates steel-safe at the small end and open them after trial results instead of trusting the paper value. The Eastman 1.65 mm blush floor applies to its copolyesters; it is not a universal constant for every thermoplastic on the market.
Every value traces to supplier documents written for their own grades. Eastman writes for Eastman polymers, DuPont writes for Zytel, Crastin, RYNITE and Minlon, and none of these bands has an ISO or ASTM standard behind it. The vestige classification in the second table leans on industry media coverage, not on resin supplier text, and the supplier guides themselves flag gate vestige allowance as a program-level decision rather than a calculated number.
What this means for your RFQ
The gate survives or dies in the RFQ stage, long before anyone inspects a part. Four inputs decide it:
- Cosmetic map: name the faces where no mark is acceptable, and name the faces where one is
- Vestige limit: state it as a number — flush or recessed, in millimetres — instead of “clean appearance”
- Exact resin grade: the grade moves the depth band, and a filled grade moves it twice
- Gate proposal sign-off: type, depth and face on paper before steel is cut, with the enlargement path confirmed
We help sourcing engineers turn those callouts into a gate decision the toolroom can machine — proposal first, steel second. Design, machining, trials and dimensional checks all run in one plant: five CNC centres with EDM and grinding feed the mould shop, eleven presses cover 80 T to 450 T of clamping force, and the largest press carries a take-out robot. Finished dimensions are verified in a bridge-CMM room, so a gate enlargement made at trial shows up in the report, not in a phone call.
Send the 3D file and the cosmetic-face map to info@hongqiangmould.com. The gate proposal travels with the quotation, and the quotation comes back within 24 hours.
Right Type | Right Depth | Right Face

Frequently asked questions
How deep should an injection moulding gate be? Start at half of the wall thickness and treat 80% as the upper edge of the band. Eastman publishes 50 to 80 percent of the wall for its copolyesters, while the DuPont nylon manual works from 45 to 75 percent, so confirm the band against the guide that matches the actual resin grade.
Do glass-filled resins need a bigger gate? Yes, the reinforced grades sit at the top of the band. DuPont recommends up to 75 percent of the wall for filled grades to limit fibre breakage and shear, and its nylon manual allows tunnel or pin gates on glass-filled nylon only above a 0.7 mm diameter.
Why does the area around the gate look hazy or shiny? That halo is gate blush, a shear-driven surface defect. Eastman links it to small gate sections and sharp transitions, and warns against gate thickness below 1.65 mm on its copolyesters. Larger gate sizes, generous radii and low-shear gating reduce the tendency.
Can a gate be enlarged after the mould is finished? Yes, and that is the intended direction. Toolmakers cut gates steel-safe at the small end of the band, then grind them open after trial results. Shrinking a gate needs welding and re-machining, so the enlargement path protects both the packing window and the trial schedule.
Jack works on the tooling and molding team at Hongqiang Mould, covering mould design, machining and trial support for export tooling programs.