We help product teams settle gate count before steel is cut, not after a short shot. On a 0.88 mm notebook cover, moving from one gate to five cut measured melt pressure from 35,000 psi to 19,200 psi and dropped the effective flow length to wall ratio from 180:1 to 120:1. Ten published resin limits show where that screen starts.
A drawing calls for a 1.5 mm wall. The resin datasheet says the grade fills easily. The first trial still leaves the far corner short, and the discussion turns to more pressure. The number that should have been checked before cutting steel is the ratio of flow path to wall, not either one alone.
Two camps argue this point. One treats flow length as a material property listed on the datasheet and reads the melt flow rate as permission to fill any geometry. The other treats every fill problem as a press problem and asks for a bigger machine.
A published gating trial shows why both positions miss. The same 0.88 mm polycarbonate cover filled at 35,000 psi through one gate and at 19,200 psi when five gates fired in sequence. Nothing changed in the resin. Only the distance the melt had to travel changed.
Four questions drove this comparison:
- What does the L/t number screen for?
- How far did one extra gate move it in a measured trial?
- Does thickening the wall beat moving the gate?
- Which inputs belong in an RFQ?
The answer that follows: gate position is a design variable, and L/t is the arithmetic that decides whether the gate belongs on the drawing or in a change order.
The screen in one paragraph
Flow length divided by nominal wall thickness gives L/t, a dimensionless number that predicts whether melt reaches the last corner before it freezes. A hot runner maker publishes maximum values at a 2.0 wall: 100:1 for PC, 170:1 for ABS, 250:1 for PP and 275:1 for LDPE. A measured notebook cover ran at 180:1 through one gate and 120:1 through five, with melt pressure falling 45 percent. In a separate study at L/t about 141, multi-stage holding cut the near-gate to far-gate width difference from 0.09 mm to 0.03 mm.
Key takeaways
- Resin screen: 100:1 for PC up to 275:1 for LDPE, all published at a 2.0 mm wall section
- Freezing law: freezing time scales with the cube of wall thickness, so a thin section closes the flow window fast
- Gate effect: five sequential gates cut measured melt pressure from 35,000 psi to 19,200 psi on a 0.88 mm cover
- Ratio shift: the same trial moved effective L/t from 180:1 to 120:1 without changing resin or part wall
- Shot rule: thin-wall work asks for at least 25 percent of barrel capacity, against a 60 oz versus 9 oz barrel contrast
- Uniformity: at L/t about 141, better holding cut far-end width scatter from 0.09 mm to 0.03 mm
Methodology
The numbers below come from three kinds of published material, and none of them is a measurement from our own presses. A hot runner manufacturer technical guide supplies the ten resin limits at a fixed wall. An industry media report records a single-gate versus sequential-gate trial on a production cover. Two peer-reviewed papers supply the pressure and dimensional results, with DOIs checked against Crossref. Where a page blocked direct retrieval from this host, the limitation is named in Limitations rather than hidden.
Arithmetic examples label themselves as arithmetic. No shop trial, sample count, customer name or machine setting has been invented to fill a gap. Site facts about our own floor appear only where they are already verified on this site.
What does L/t actually screen before steel is cut?
L/t divides the longest distance melt travels from gate to the last point of fill by the wall thickness along that path. A high ratio means a long, thin channel; the frozen skin grows inward from both walls and the open core narrows before the cavity fills. The guide below states its values apply to a 2.0 mm wall section and that the maximum falls as walls get thinner.
| Resin | Maximum L/t at 2.0 mm wall |
|---|---|
| LDPE | 275:1 |
| PP | 250:1 |
| HDPE | 225:1 |
| PS | 200:1 |
| ABS | 170:1 |
| PA | 150:1 |
| POM | 150:1 |
| PMMA | 130:1 |
| SAN | 120:1 |
| PC | 100:1 |
Read the table as a starting line. A ratio under the resin value leaves room for error; one over it demands a gate change or a fill study.
That screen is not a guarantee. Gate style, melt and mould temperature, texture and venting all move the practical limit.
What changed when a fifth gate fired?
The notebook cover trial used one centre gate and one near each corner, all on a 0.88 mm polycarbonate part. The single-gate run needed pressure above what an ordinary press delivers. Sequential firing let the centre gate start the fill and the outer gates take over as the front arrived, shortening each flow path without leaving weld lines on the cover.
| Measured item | Single gate | Five sequential gates |
|---|---|---|
| Wall thickness | 0.88 mm | 0.88 mm |
| Effective L/t | 180:1 | 120:1 |
| Melt pressure | 35,000 psi | 19,200 psi |
| Fill time | 0.45 s | 1.08 s |
| Cycle time | about 25 s | 21 s |
| Weld lines | none | none |
Same wall, same resin, one third less L/t. Pressure followed the geometry, not the press rating.
Adding gates bought margin. Slower fill still produced a shorter cycle because the machine worked at lower pressure.

Does a thicker wall beat a second gate?
Sometimes, but the cost lands in a different place. Thickening a wall adds resin to every part and lengthens the cooling phase, which is usually the longest part of the cycle. Moving a gate changes one plate of the tool. The arithmetic below uses the PA limit of 150:1 from the guide above; it is a calculation, not a shop trial.
| Case | Longest path / wall | L/t |
|---|---|---|
| 300 mm path at 2.0 mm wall | 300 / 2.0 | 150:1 |
| Same 300 mm path at 1.5 mm wall | 300 / 1.5 | 200:1 |
| Centre gate, 150 mm path at 1.5 mm wall | 150 / 1.5 | 100:1 |
Halving the path does what thickening cannot do cheaply. The wall stays light and the ratio returns inside the screen.
Every extra millimetre of wall is paid for on every shot. A gate move is paid for once.

What does a high ratio do after the cavity fills?
L/t also predicts how evenly the part holds dimension from gate to far end. An International Journal of Heat and Mass Transfer study used a part at L/t about 141 and tracked the pressure left in the cavity at the end of packing. Multi-stage holding reduced the residual difference from 48.7 MPa to 12.5 MPa, and the near-to-far width gap fell from 0.09 mm to 0.03 mm.
A Polymers study compared two tools running the same highly filled polycarbonate. The tensile bar tool had L/t 121 and needed 198.8 MPa; the box tool had L/t 66 and needed 102.6 MPa. The pressure ratio of 1.94 sat close to the L/t ratio of 1.83. Gate area also differed between the tools, so the paper does not claim L/t as the only cause.
These results change what an RFQ should ask. A ratio that fills may still leave a part that drifts after ejection.
Limitations
Test conditions versus the shop floor. The resin table assumes a 2.0 mm wall section and states that limits fall as walls thin. The five-gate result comes from one 0.88 mm cover on a high-pressure machine with a sequential controller. A general-purpose press, a textured face or a longer runner will not repeat those numbers. Treat every published limit as a screen with margin, not a pass mark.
Third-party data sources. PlasticsToday, ScienceDirect and MDPI pages returned 403 to direct retrieval from this host; their text was verified through search-index content, and the two journal DOIs were checked against Crossref. The Mastip guide was retrieved and read as a PDF. No figure here is presented as our own measured trial. Surface finish can also reverse expected flow behaviour: one spiral-flow study on polycarbonate found up to 3 percent longer flow on rougher cavities than on polished ones.
What this means for your RFQ
Our own floor runs eleven presses from 80 T up to a 450 T JSW with a take-out robot, with five CNC machines, EDM, grinding and a bridge CMM in the metrology room. That setup is why our team checks gate position against wall thickness at DFM, before steel is ordered. It is also why we ask for the longest flow path, not just the part length: a cover with ribs around a boss can hide twice the distance the outline suggests.
L/t is the number that decides whether the gate belongs on the drawing or in a change order.
Send a 2D or 3D file with the resin grade, nominal wall, longest flow path and proposed gate location to sales@hongqiangmould.com. A quotation reaches you within 24 hours, with the gating assumption written down so it can be challenged. From first sketch to production tool, one team handles the review.
Checked | Gated | Quoted
Frequently asked questions
What is a good L/t ratio for injection moulding? Published maximum L/t ratios start around 100:1 for polycarbonate and reach 275:1 for LDPE, based on a 2.0 mm wall section from a hot runner maker guide. Treat those values as a first screen, not a guarantee. Wall thickness, gate design, venting and resin grade all move the real limit.
How does adding a gate change L/t? Each gate shortens the longest path the melt must travel. In one published notebook cover trial, five sequential gates cut the effective L/t from 180:1 to 120:1 on a 0.88 mm wall. Melt pressure fell from 35,000 psi to 19,200 psi. Weld lines stayed out because the gates fired in sequence, not all at once.
Does a thicker wall fix a short shot? A thicker wall raises the L/t headroom, but it also adds material cost and cooling time. On a 300 mm flow path, moving from a 2.0 mm to a 2.5 mm wall drops L/t from 150:1 to 120:1. Moving the gate can reach the same number without adding resin to every part.
Who should supply the L/t data in an RFQ? Send the resin grade, nominal wall, longest flow path and proposed gate location. Our tooling team reviews those four items before steel is ordered and returns a quotation within 24 hours. Published resin tables give a screen; a fill study checks the result on parts with variable walls or tight cosmetic faces.