Hongqiang Mould logoHongqiang Mould

A sink EDM leaves a 3.7-53 µm white layer on H13, and no CMM report will show it (3 studies)

A sink EDM leaves a 3.7-53 µm white layer on H13, and no CMM report will show it (3 studies)

← Back to Blog · A sink EDM leaves a 3.7-53 µm white layer on H13, and no CMM report will show it (3 studies)

We help mould buyers judge whether a spark-eroded cavity is production-ready. Three peer-reviewed studies put the EDM white layer between 3.7 and 53 µm deep on die steels, with a skin up to about 1.9 times harder than the steel beneath it. This article shows where the layer comes from, why it polishes badly, and how much steel has to come off.

The numbers in one paragraph: the white layer is re-solidified steel, melted by the spark and quenched in the dielectric. Measured depths run from 3.72 µm at a 1 A finishing burn to 53.2 µm at 500 µs pulses on H13-type steel. The skin tests 800–920 HV where the parent metal sits near 500 HV, and the band 12 µm further down drops to 280–390 HV. Depth follows pulse-on time and current, not voltage. A CMM sees none of it.

Every cavity we cut passes over the EDM bench at some point. Deep ribs, sharp shut-offs and slots too narrow for a cutter all end up spark-eroded, and the steel that comes off the machine looks finished. It is on size, and it photographs like done work.

Opinions split right there. One camp treats the as-EDM surface as a finish in its own right and sends the plates to assembly. The other camp stones every burned face on principle, quoting hand-polishing hours that no drawing ever asked for.

The real problem sits between those habits. The layer the spark leaves behind is a few microns of brittle, over-hard steel that routine checks never look at. A CMM report comes back clean because a CMM reads geometry, not metallurgy. The layer shows up later: orange peel under the polisher, a chipped edge on first articles, a crack line across a shut-off.

Three questions drove the comparison:

  • How deep is the layer at finishing and roughing currents?
  • What does the hardness profile under the surface look like?
  • How much steel has to come off before the cavity is safe?

Short version: the layer is thin when the burn is gentle, it is harder than the steel under it, and removing it is a planning decision rather than an accident.

Key takeaways

  • Depth window: 3.72 µm at the gentlest tested burn; 53.2 µm at 500 µs pulses on H13-type steel.
  • Hardness flip: 800–920 HV at the surface over a 280–390 HV band at 12 µm depth.
  • The voltage trap: current, pulse-on and pulse-off times move the depth; voltage does not.
  • Removal rule: stone past the layer, not down to it — measured depth plus a few microns of margin.
  • Inspection gap: CMM reads geometry only; the layer needs a cross-section and an etch.

Methodology

This breakdown rests on published metallography, on arithmetic we ran ourselves, and on the way our own tool room sequences the work. Three peer-reviewed studies anchor the measured figures, all of them on die-sinking EDM of SKD61 / H13-type steel with copper electrodes: a 2021 Taguchi analysis in the International Journal of Engineering, a 2021 microstructure study in Metals, and a 2013 cavity-specific study in Revista Matéria.

Layer depths and hardness values are measured figures from those papers. Two numbers are ours: the HRC-to-HV conversion for the parent steel, and the exponent linking pulse-on time to layer depth. Both are calculations from published data and are marked as such in the text. Shop sequencing statements come from our bench, where copper electrodes are burned into pre-hardened and hardened die steels before stoning and CMM checks. Lab coupons are not production cavities, and that gap runs in both directions.

How thick does the layer get?

Depth tracks the energy of each pulse. A gentle finishing burn leaves a film measured in single microns; a heavy roughing condition leaves tens of microns of re-cast steel.

Condition (die-sinking, copper electrode)SteelWhite layer depthSource
1 A, 30 V, 50 µs on / 12 µs offSKD613.72 µmIJE 2021
Water + nitrogen dielectric, 100 µs pulsesH13 (SKD-61)31.0 ± 4.6 µmMetals 2021
Water + nitrogen dielectric, 500 µs pulsesH13 (SKD-61)53.2 ± 5.5 µmMetals 2021
Wire EDM, low energyMonel 4002.55 µmMetals 2021
The last row is a nickel-copper alloy, listed as a low-energy reference point rather than a steel value.

From a skim burn to a long-pulse condition, the range spans a factor of fourteen. Depth follows pulse energy, so the finishing condition you specify decides the cleanup.

Depth alone does not settle the case, though. The 2013 cavity study found microcracks in the layer under severe conditions, running perpendicular to the surface, and cracks do not care how thin the film is.

Two moulded housings with internal slots and rib packs, the kind of steel details cut by sinker EDM
Internal slots and rib packs like these are the geometry that ends up spark-eroded, microns at a time.

Why does the hardest skin polish the worst?

The white layer is harder than the steel under it, and the drop-off is steep. The Metals study measured 800–920 HV0.025 at the surface of an H13-type steel, then 280–390 HV0.025 at 12 µm depth. Convert the usual 48–52 HRC parent hardness with ASTM E140 tables and the bulk sits near 480–540 HV, our calculation.

ZoneHardnessReading
White layer at the surface800–920 HV0.0251.5–1.9× the parent steel
12 µm below the surface280–390 HV0.02525–40% softer than the parent steel
Parent steel at 48–52 HRC≈480–540 HVConverted from HRC, our calculation
Hardness figures from the Metals 2021 study; the parent-steel row is a conversion, not a measurement.

A stone glazes on the hard skin, then bites fast once it breaks through into the softened band. That uneven cut is the orange peel polishers complain about. The same brittleness chips edges on thin shut-off steel during handling.

The 2013 paper draws the same profile in three zones: a white layer above 800 HV, a quenched heat-affected zone below it, then parent metal. Conversion tables are approximations, so treat the ratio as the finding and the digits as guidance.

Which settings actually move the depth?

The Taguchi study ranked four variables against recast thickness on SKD61. Three of them matter. One does not.

VariableEffect on white layer depthEvidence
Discharge current (Ie)SignificantTaguchi, IJE 2021
Pulse-on time (Ton)Significant, dominantIJE 2021; Revista Matéria 2013
Pulse-off time (Tof)SignificantTaguchi, IJE 2021
Open-circuit voltage (Ue)Not significantTaguchi, IJE 2021
Cavity depth, electrode geometryAlso shift resultsRevista Matéria 2013
Significance as reported by each study; the two papers used different test rigs.

In the Metals dataset the depth scales with about the cube root of pulse-on time. That exponent, 0.34, is our calculation from the two measured points. Doubling pulse-on adds roughly 26% layer depth. The cheaper lever stays the same either way. Finish with a low-energy burn and let the stone remove microns, not tenths.

How much steel has to come off?

Clearing the layer means removing more than its thickness, because the band under it is over-tempered and damaged too. The table below is our engineering recommendation for planning, with the layer depths tied back to the studies above.

Burn conditionLayer to clearRemoval allowance (our recommendation)Typical tooling
Fine skim burn≈4 µm5–10 µmFine stone, then paper
Medium finishing burn10–20 µm (industry-typical)15–25 µmStone, paper, diamond paste
Roughing burn31–53 µmLayer depth plus margin; plan as re-machiningDiamond stoning, grinding or re-cut
Allowances are planning numbers, not standard values; measure the burns on your own steel.

A skim burn cleans up in minutes at the bench. A roughing burn leaves more than fifty microns of glass-hard film. Clearing that is a machining operation, and the hours show up in the quote. The grades above that surface carry their own price, which our SPI finish and polishing-step breakdown covers in detail.

One boundary belongs here. An allowance measured on a flat coupon underestimates a deep pocket, because the 2013 study showed layer thickness and cracking vary with cavity depth and electrode geometry.

Limitations

Coupon studies and production steel disagree in one direction: real cavities add deep pockets, tight flushing and curved shut-offs, and every one of those thins or thickens the layer locally. The measured depths above come from flat, well-flushed samples, so treat them as mid-points rather than guarantees.

Every depth and hardness figure here comes from three university studies, not from our press floor. We did not section a cavity for this article. The tested grades, SKD61 and H13-type steels, cover most but not all mould steels, and the removal allowances are our planning numbers rather than lab results.

What this means for your RFQ

We help sourcing engineers turn surface integrity into drawing notes a tool room can price. Name the finishing burn energy on the drawing. Ask how the burned faces will be cleared. Treat the stoning allowance as a line item, not as goodwill, because it is cheaper to remove the layer while the steel is still on the bench than after first articles. From prototype to production, the sequence runs burn low, stone deep, record it.

Send your 3D drawings to info@hongqiangmould.com and a quotation that separates EDM, stoning and polishing line by line comes back within 24 hours. Documented | Stoned | On Size.

Frequently asked questions

Does every EDM pass leave a white layer on the cavity? Yes. Each spark melts a film of steel that re-solidifies on the surface, and the cited studies measured that recast layer at every condition tested, from 3.72 µm at a gentle burn to 53.2 µm at long pulses. Automatic finishing circuits thin the layer but do not remove it.

Can a CMM report catch a bad EDM surface? No. A CMM measures geometry, and the white layer sits inside the tolerance envelope. Detecting it takes a metallographic cross-section with etching, the method the cited studies used. If surface integrity matters on your project, ask for it as a documented step before the mould ships.

Is an EDM finish acceptable as the final cavity surface? For matte texture faces, yes, and many housings call for exactly that look. For gloss or diamond-grade finishes, no: the burned skin resists polishing and chips at edges. Stone past the layer first, then work the grade ladder your drawing names.

Does wire EDM leave the same kind of layer? Yes, the metallurgy is the same. The low-energy wire measurement in the Metals study gave 2.55 µm on a nickel-copper alloy, and low-energy steel burns sit near the fine figures in the first table. Treat wire-cut shut-offs like sinker work: low energy last, then stone.

Jack works on the tooling and molding team at Hongqiang Mould, a mould shop in China that builds injection moulds and runs production moulding on 11 presses from 80 to 450 T. He writes about the numbers behind tooling decisions: clamp force, cooling, ejection and the tolerance stack that decides whether a part assembles.

Sources

Phan, N. H., et al. “Influence of Process Parameters on the Microstructural Characteristics and Mechanical Properties of Recast Layer Thickness Coating on Die Steel Machined Surface after Electrical Discharge Machining.” International Journal of Engineering, vol. 34, no. 5B, 2021, doi:10.5829/ije.2021.34.05b.24.

“Sub-Microstructure of Surface and Subsurface Layers after Electrical Discharge Machining Structural Materials in Water.” Metals, vol. 11, no. 7, 2021, article 1040, doi:10.3390/met11071040.

Zeilmann, Rodrigo Panosso, Thiago Vacaro, Fernando Moreira Zanotto, and Mariana Czarnobay. “Metallurgical Alterations in the Surface of Steel Cavities Machined by EDM.” Revista Matéria, vol. 18, no. 4, 2013, doi:10.1590/S1517-70762013000400014.


Technical Guides

Browse all technical guides →

/* data-no-optimize is REQUIRED: LiteSpeed rewrites plain inline scripts to type="litespeed/javascript", which browsers never execute. This site's existing inline scripts already use the same attribute. */