Hongqiang Mould logoHongqiang Mould

Glass-Filled Nylon Shrinks 3× More Across Flow

Glass-Filled Nylon Shrinks 3× More Across Flow

← Back to Blog · Glass-Filled Nylon Shrinks 3× More Across Flow

A 30 % glass-filled nylon grade shrinks about 0.25–0.3 % along the flow and 0.75–1.1 % across it, according to three manufacturer data sheets. That 2.7–3.7× gap breaks the usual plan of scaling steel by one percentage. The cavity needs two allowances, and the RFQ has to say which direction each one belongs to.

The RFQ says “PA6-GF30, shrinkage 0.3 %”. The buyer assumes one number describes the part. Steel gets cut with a single scale factor, the first samples measure long in width and short in length, and the discussion turns to packing pressure.

Two positions show up at that point. One side insists the datasheet number is wrong and asks for a different grade. The other side adds stock to every wall, then argues about which cavity to shim during sampling.

Neither side has read the row beside the number. The sheets publish shrinkage in two axes: one parallel to flow, one normal to it. Glass fibres line up with the moving melt, and the two numbers part ways. A 0.3 % figure usually describes the direction the fibres point, not the direction the part fails.

Four questions shaped this comparison:

  • How wide is the split between the two axes in published grade data?
  • What does that split become in millimetres on a real span?
  • Why does adding 30 % glass make the two axes behave so differently?
  • Which fields belong on the drawing before a quote is requested?

The answer in advance: three data sheets put the cross-flow allowance at roughly three times the along-flow allowance, and the same BASF grade is published with two different pairs depending on which sheet the buyer holds.

The split in one paragraph

BASF publishes its PA6-GF30 grade B3WG6 GP at 0.25 % parallel and 0.75 % normal. A second BASF sheet for the same trade grade lists 0.3 % and 0.8 %. DuPont publishes PA66-GF30 Zytel 70G30HSLR at 0.3 % parallel and 1.1 % normal. Those pairs give ratios of 3.0, 2.7 and 3.7. On a 100 mm span the first pair means 0.25 mm in flow and 0.75 mm across it, a 0.50 mm difference that a single scale factor cannot produce. BASF also lists thermal expansion of 25 versus 90 ×10⁻⁶/K for that grade, so the two axes keep diverging after the part leaves the tool.

Key takeaways

  • Flow axis: 0.25 % for BASF B3WG6 GP, 0.3 % for DuPont Zytel 70G30HSLR
  • Cross-flow axis: 0.75 % and 1.1 % on the same two grades, a 2.7–3.7× split
  • Span effect: 0.50 mm and 0.80 mm of difference across a 100 mm reference span
  • Sheet conflict: one BASF trade grade appears as 0.25/0.75 and as 0.3/0.8 in two documents
  • Thermal follow-through: 25 versus 90 ×10⁻⁶/K expansion keeps the axes apart in service

Methodology

Three manufacturer data sheets supply every shrinkage figure below. The BASF sheet for Ultramid B3WG6 GP BK23210 was downloaded from BASF’s own document server. A separate BASF B3WG6 sheet was obtained through ALBIS, a resin distributor. The DuPont sheet for Zytel 70G30HSLR NC010 was read from a distributor-hosted copy of the manufacturer document. Each file was opened locally and the processing rows were extracted from the text layer, not from a summary page.

All three sheets cite ISO 294-4 for moulding shrinkage, and the two BASF sheets also cite ISO 2577. The field names are “parallel” and “normal” or “transverse”; both describe the axis across the flow relative to the gate. Millimetre allowances in the second table are arithmetic on a 100 mm reference span, calculated as percentage × span ÷ 100. They are not measurements of a moulded part.

The shop context is real but limited. Hongqiang builds tooling in house, runs 11 presses between 80 and 450 T, and checks multi-cavity plate assembly before trials. No fibre-orientation scan and no in-house shrinkage study exists here, so nothing in this article is presented as our own material test.

What Do Three Manufacturer Sheets Actually Publish for Directional Shrinkage?

The parallel number stays near 0.3 % across all three documents. The cross-flow number moves between 0.75 % and 1.1 %, which is where the spread lives.

Grade and documentParallel to flowNormal to flowSplit
BASF Ultramid B3WG6 GP BK23210, PA6-GF300.25 %0.75 %3.0×
BASF Ultramid B3WG6 via ALBIS, PA6-GF300.3 %0.8 %2.7×
DuPont Zytel 70G30HSLR NC010, PA66-GF300.3 %1.1 %3.7×

The two BASF rows describe one trade grade and disagree by 0.05 points in both axes. Name the data sheet in the RFQ.

The DuPont row is the widest split. A glass-filled PA66 part will not respond to one shrink factor.

What Does the Split Become in Millimetres on a 100 mm Span?

Percentages are hard to argue about at a bench. Converting them to millimetres on a fixed span shows the size of the decision in steel.

GradeAlong flow on 100 mmAcross flow on 100 mmGap between axes
BASF B3WG6 GP0.25 mm0.75 mm0.50 mm
DuPont Zytel 70G30HSLR0.30 mm1.10 mm0.80 mm

A 0.50 mm gap is not a trimming allowance. It is two different cavity sizes in two directions.

Both rows are calculated, not measured. Real spans, gates and wall sections change the local result.

Why Does Adding Glass Fibres Separate the Two Axes?

Fibres travel with the melt and align along the path from gate to the last corner to fill. In that direction the stiff glass carries a share of the load, so the cooled part gives back less length. Across the flow the matrix controls contraction, and the same part gives back more width.

BASF’s sheet makes the same point in thermal expansion rather than moulding shrinkage. Its PA6-GF30 grade lists 25 ×10⁻⁶/K longitudinally and 90 ×10⁻⁶/K transversely between 23 and 55 °C. That ratio is 3.6, close to the 3.0 shrinkage ratio. A part dimensioned at room temperature therefore keeps opening the same directional gap when the assembly warms up.

Fibre alignment also changes from skin to core and from one flow region to another. This is why a gate move can alter width while barely touching length. The datasheet pair is a starting allowance; the gate position decides how closely the part follows it.

Multi-cavity mould plate with cooling ports and inserts checked on the fitting bench

How Do You Put a Two-Axis Shrink Requirement on an RFQ?

Replace the single shrinkage line with fields that name a direction and a document. The block below uses the BASF GP sheet as an example.

FieldValue to state
Resin and data sheetPA6-GF30, Ultramid B3WG6 GP BK23210, BASF sheet
Flow referenceGate position drawn on the part, with the longest fill path marked
Along-flow allowance0.25 %, taken from the parallel row
Across-flow allowance0.75 %, taken from the normal row
Cavity steelTwo scale factors in the tool drawing, one per axis
Controlling dimensionBuyer names which axis carries the tight tolerance

Six fields replace one line and remove most of the guesswork. The gate mark matters because the words parallel and normal have no meaning without a flow path.

Our team reviews those six fields before steel is ordered. A drawing that names only a grade gets a question back, not a scale factor.

Limitations

Test bars are not production parts. ISO 294-4 shrinkage comes from standard specimens with a straightforward flow path; a housing with ribs, bosses and side actions builds local orientation that no single datasheet row describes. The millimetre figures here are arithmetic on a chosen span, so they scale with the actual dimension and with the local flow.

The three documents come from two resin makers, and one DuPont sheet is read from a distributor copy rather than a manufacturer host. The two BASF values disagree, which is itself a warning about treating any one sheet as a fixed specification. LANXESS sheets were not reachable from our connection and are excluded.

What this means for your RFQ

We help tooling teams hold two allowances instead of pretending one will do. Send the resin grade, the nominal wall and the flow direction marked on the part, and name the tightest tolerance axis. Our reviewers map those inputs to cavity steel before the first cut, using the 80–450 T press range to check that the tool and the expected output fit together.

Quotation within 24 hours of receiving 2D or 3D drawings. Direction | Allowance | Evidence.

Frequently asked questions

Why does glass-filled nylon need two shrink numbers? Fibres align with melt flow. Shrinkage along that alignment is restrained by the glass, while shrinkage across it comes mostly from the polymer matrix. BASF lists 0.25 % parallel against 0.75 % normal for one PA6-GF30 grade. One factor cannot describe both directions on the same cavity.

Which datasheet value should I use for a glass-filled PA part? Use the sheet tied to the exact grade and supplier, then write its name on the drawing. Two BASF documents for the same PA6-GF30 trade grade publish 0.25/0.75 and 0.3/0.8. A grade name alone does not identify which pair the toolmaker should cut.

Does a thicker wall reduce directional shrinkage? Thicker sections hold heat longer and change both packing and fibre orientation, so the two axes do not move together. The data sheet values were measured on standard bars, not on thick ribs. Treat wall changes as a reason to recheck the allowance, not as a way to remove the split.

Can packing pressure correct a cross-flow dimension? Packing can move a dimension, but it acts on the whole filled path and can distort the axis already close to target. When the two allowances differ by 0.5 mm across 100 mm, correcting steel is cleaner than forcing the part with pressure. Measure both axes before changing either.

Jack works on the tooling and molding team at Hongqiang Mould, covering mould design, machining and trial support for export tooling programs.


Technical Guides