Mould temperature is a cavity-surface target, not a chiller setting. Three supplier sheets put polypropylene homopolymer at 10–30 °C, ABS at 30–80 °C and PA6 at 40–60 °C. A 504-hour test on one polypropylene grade shows the tool temperature also moves final shrinkage by 0.11 points and keeps the part drifting for three weeks.

A mould drawing arrives with a material line and a tolerance block. Nobody writes the tool temperature on it. The moulder sets the chiller to whatever the last job used, parts come out, and the dimension report gets signed on a tool that is still climbing toward steady state.

Two camps own this argument. One camp reads “mould temperature 40–60 °C” off the resin sheet and treats the chiller setpoint as that figure. The other camp files temperature under machine settings, so it lives with the process engineer and never reaches the tool drawing at all.

Both camps skip the same distinction. The datasheet figure is a cavity surface value measured under ISO 294 conditions. The chiller figure is the medium entering the circuit. Steel thickness, inserts, baffles and the distance from circuit to cavity all sit between the two, and when they are confused, a part that measured in tolerance at 24 hours walks out of tolerance over the following weeks.

Four questions drove this comparison:

  • What do three supplier sheets actually publish for tool temperature?
  • How much does tool temperature move shrinkage, in a controlled test?
  • Which number belongs on the RFQ, and in what units?
  • Which checks catch a temperature mistake before sign-off?

The short version: the published window is a processing envelope, not a dimension target, and the RFQ needs a surface value with a tolerance before steel is ordered.

The gap in one paragraph

Three commodity grades, read from their own product data: polypropylene homopolymer 10–30 °C, ABS 30–80 °C, PA6 40–60 °C. The top of the polypropylene window and the top of the ABS window sit 50 °C apart. In a 504-hour polypropylene study, raising the tool from 20 °C to 80 °C lifted shrinkage at 24 hours from 1.44 % to 1.55 %, and both sets kept shrinking through week three, ending at 1.56 % and 1.63 %. Annealing erased the gap. So the tool temperature decides where a part lands inside its shrinkage band, and the clock decides when.

Key takeaways

  • Window spread: 10–30 °C for PP homopolymer, 30–80 °C for ABS, 40–60 °C for PA6, each from its own supplier sheet
  • Tool effect at 24 h: 60 °C more surface temperature added 0.11 shrinkage points on one PP grade
  • Drift after trial: 0.05 and 0.04 points still moving between 168 h and 504 h at the two tool temperatures
  • Equaliser: 24 h at 140 °C brought both sets to roughly 2 %, so the difference is timing, not permanent geometry
  • RFQ input: one cavity surface value per resin plus a tolerance band, quoted back within 24 hours

Methodology

The evidence base is four documents, not a survey. Three are current product data sheets from the resin suppliers themselves: Borealis HJ325MO for polypropylene homopolymer, INEOS Styrolution Terluran GP-22 for ABS, BASF Ultramid B3K for PA6. Each processing block follows ISO 294 field names, so mould temperature, melt temperature and moulding shrinkage sit in the same rows across suppliers. The fourth document is a peer-reviewed study by Kościuszko, Marciniak and Sykutera in Materials 14(1):22 (2020), which moulded polypropylene tensile bars at two tool temperatures, conditioned them for 504 hours at 23 °C, then annealed them for 24 hours at 140 °C.

Two measurement notes matter for reading the numbers below. Shrinkage in the supplier sheets is a typical value for uncoloured resin, tested on standard bars, not on a customer part. Shrinkage in the study is linear shrinkage calculated from specimen length after defined conditioning intervals, so the time stamps are part of the result, not a footnote.

Our own contribution is a feasibility screen, not a measurement campaign. Tooling is built in house here, and the press list spans 11 machines between 80 and 450 T. The resin set below covers what those machines see most weeks. No cavity-surface data from our floor appears in the tables, and none is implied.

What Do Three Supplier Datasheets Actually Say About Mould Temperature?

Read side by side, the three sheets split into three separate bands. Polypropylene wants a cold tool. ABS tolerates a wide middle. PA6 sits in a narrow band just above the ABS floor.

ResinGrade and sourceMould temperatureMelt temperatureMoulding shrinkage
PP homopolymerBorealis HJ325MO10–30 °C210–250 °C1–2 %
ABSINEOS Terluran GP-2230–80 °C220–260 °C0.4–0.7 %
PA6BASF Ultramid B3K40–60 °C250–270 °C0.65 % constrained, 0.75 % parallel

The widest window belongs to ABS at 50 °C of travel. Polypropylene and PA6 each get 20 °C. One shared water temperature already sits outside one of these windows.

The INEOS sheet adds a processing note. Higher surface temperature raises gloss and weld-line strength within gate and geometry limits. Gloss is therefore a temperature readout as much as a steel polish readout.

Why Does 60 °C More Tool Temperature Move Shrinkage Only 0.11 Points?

Because the first 24 hours are not the whole story. The Polish study moulded the same polypropylene at 20 °C and at 80 °C, then measured length at fixed intervals instead of once.

Mould temperatureShrinkage at 24 hAt 168 hAt 504 hAfter 24 h annealing at 140 °C
20 °C1.44 %1.51 %1.56 %about 2 %
80 °C1.55 %1.59 %1.63 %about 2 %

Two readings follow from the table. The hot tool starts 0.11 points ahead and stays ahead, so the rank never flips.

The second reading is the one that bites. Between week one and week three, the cold-tool parts moved another 0.05 points and the hot-tool parts another 0.04. A report signed at 24 hours reads tighter than the same parts three weeks later.

The study attributes the movement to secondary crystallisation: the amorphous phase keeps converting after demoulding, and density rises with it. Its density measurements put annealed samples of both sets at 0.911 g/cm³ and 70.6 % crystallinity, which is why annealing collapses the difference. Crystallinity gain over the 504 hours is reported as 2.2 % at the cold tool against 0.9 % at the hot tool.

Bench-top force tester checking a moulded sample at the inspection station

The practical consequence: tool temperature decides which side of a shrinkage band a part sits on, and conditioning time decides how far it travels. Neither number is stable on its own.

How Do You Turn a Datasheet Window Into a Number on the RFQ?

Write the surface value, not the chiller value. The table below is the block we ask buyers to fill in before a tool drawing is released, with the polypropylene case filled out as an example.

FieldValue to state
Resin and gradePP homopolymer, HJ325MO class
Cavity surface target20 °C, the middle of the published 10–30 °C window
Tolerance on surface±3 °C, common shop practice rather than a standard
Where it is measuredCore and cavity inserts, contact probe, after the tool reaches steady state
Cooling medium12–18 °C water, industry-typical for polypropylene, not a fixed rule
Who owns the numberMoulder states the surface; toolmaker sizes circuits to deliver it

Three of those rows do the heavy lifting. The surface value prevents a chiller argument at trial. The tolerance band tells the toolmaker how much circuit authority is needed. The measurement point removes the usual ambiguity about whether the probe was on steel or in a hose.

Baffles, bubblers and insert geometry all change what a given circuit delivers at the surface. So the number belongs in the tool specification, while circuit layout is still open. The trial report is too late.

Which Checks Catch a Mould Temperature Mistake Before Sign-Off?

Five checks, in the order they catch problems:

  • Surface before dimensions. Probe core and cavity at steady state, then measure the part. A cold tool produces a tight first report that will not hold.
  • Two time stamps. Report dimensions at 24 hours and again at 168 hours. The published drift is small per week but additive.
  • Gloss against the standard. A dull patch beside a gate often tracks surface temperature, not steel polish, so check temperature before repolishing.
  • Circuit flow and return difference. A restricted circuit shows up as a temperature spread across the plate before it shows up as a dimension.
  • Resin change review. Swapping PP for PA6 in the same tool moves the target from 20 °C to 50 °C, which is a circuit and medium decision, not a setpoint tweak.

None of these checks needs new equipment. A contact probe, a flow meter and a measurement schedule cover all five.

Limitations

Laboratory bars and production parts behave differently. The 504-hour study used standard tensile specimens with a simple geometry, so its drift figures describe a material trend rather than a specific housing, lid or bracket. Thick sections, long flow paths and heavy rib grids will move on their own schedule.

The four documents come from three suppliers and one research group. Each carries its own test conditions, and the supplier shrinkage values are typical figures for uncoloured resin, not guarantees for a coloured or filled compound. A different grade within the same family can shift the window by several degrees.

What this means for your RFQ

Fixing the tool temperature on the drawing costs a line of text. Fixing it after the circuit is drilled costs a strip-down. We help buyers settle that number while the cooling layout is still open, so the trial confirms a decision instead of reopening one. Send the resin grade, the wall section and the tolerance that matters, and state whether the tool will run cold or warm. Our tooling team then checks circuit capacity against the target and confirms press fit across a machine list that runs from 80 to 450 T.

Quote back within 24 hours of receiving 2D or 3D drawings. Measured | Repeatable | On Schedule.

Frequently asked questions

What mould temperature should I write on a mould drawing? Write the cavity surface target, not the chiller setpoint, and add a tolerance band. The published windows are 10–30 °C for polypropylene homopolymer, 30–80 °C for ABS and 40–60 °C for PA6. The toolmaker then sizes circuits and chooses a medium that delivers that surface value.

Does a hotter tool always make parts shrink more? For the polypropylene grade tested, yes within the band. A tool at 80 °C gave 1.55 % at 24 hours against 1.44 % at 20 °C, and stayed ahead at 1.63 % versus 1.56 % after 504 hours. Annealing both sets at 140 °C brought them to roughly 2 %.

Why do two suppliers quote different windows for the same resin? Grade, additive package and intended process differ, and the window edges follow the test standard in use, usually ISO 294. A homopolymer with a 1–2 % shrinkage band tolerates a cold tool. A glass-filled or thick-section grade often needs a warmer surface to fill and hold gloss.

How long should dimensions be tracked before approval? Measure at 24 hours and again at 168 hours, then compare both sets to the drawing. The published test still showed 0.04 to 0.05 points of movement between week one and week three. Parts held for a customer audit should follow the same schedule.

Jack works on the tooling and molding team at Hongqiang Mould, covering mould design, machining and trial support for export tooling programs.


Technical Guides