We help buyers specify the moisture state that decides which size a nylon part delivers, before the first CMM report is written. A PA66 part leaves the press dry, then absorbs about 2.7% moisture at ordinary room humidity and 8.5% when soaked, according to ISO 62 and ASTM D570 data published by DuPont and LANXESS. Along the way its stiffness drops to well under half, and its size settles into a state the drawing has to name.

A nylon housing that measured perfectly on our bridge CMM at the press can measure differently a few days later at the assembly plant. In most cases that gap is not a quality escape. It is water.

Moulded sample clamped in a bench-top force tester at the inspection bench
First-article checks at the inspection bench record the dry-as-moulded state.

Moulders quote dry-as-moulded numbers because that is the state of the part when it leaves the machine. Designers size assemblies around room-conditioned behaviour because that is the state of the part in service. Both sides read the same datasheet, and both walk away right.

The datasheet carries both columns, yet the drawing usually names neither state.

We set out to answer four questions using published resin-maker documents rather than workshop impressions:

  • How much water does PA66 take on at ordinary room air, and how fast?
  • What does that water do to stiffness and toughness?
  • Which polyamide grades move least?
  • What belongs on the drawing and in the RFQ so that both measurement states are explicit?

The short answer: 2.7% water at 50% relative humidity, less than half the dry stiffness, and a one-line conditioning note that costs nothing to add.

Key takeaways

  • 2.7% water in room air: PA66 reaches equilibrium at 23 °C and 50% RH with 2.7–2.8% moisture (ISO 62, DuPont and LANXESS data); it holds 8.5–9.0% when saturated in water.
  • Stiffness falls 61%: the tensile modulus of Zytel 101L drops from 3100 MPa dry to 1200 MPa at 50% RH — same grade, same temperature, different water.
  • Strength down, stretch up: yield stress falls from 83 to 53 MPa while yield strain rises from 4.5% to 25%.
  • Days, not hours: a 2 mm PA6 wall reaches roughly 2.2% moisture in about 100 hours of storage at 23 °C and 50% RH.
  • Toughness pays back: notched Izod climbs from 53 to 112 J/m, and the allowable snap-fit strain rises from 4% dry to 6% conditioned.
  • PA12 and PA610 move least: 0.8% equilibrium and 1.5% saturation in the LANXESS table — a third of the uptake of PA6.

Methodology

Every number in this article comes from three published documents, not from our own environmental testing: the DuPont Zytel 101L NC010 datasheet, the LANXESS conditioning document for Durethan mouldings, and the DuPont general design principles manual for engineering polymers. Our shop runs PA on presses from 80 to 450 T and measures parts on a bridge CMM, but we have not run humidity-chamber ageing studies, and nothing here should be read as our own measurement.

We read the datasheet columns as printed and the LANXESS storage-time curves as approximate values, because that document publishes them as chart annotations. Where the two resin makers give the same property, we quote both figures. The absorption standards differ in specimen: ISO 62 uses a thin plate, ASTM D570 a 3.2 mm disc, so 24-hour values between the two methods are not interchangeable. The documents were accessed through official distributor mirrors because the original portals were unreachable from our network at the time of writing; links appear in the text.

Why does a nylon part change size after it leaves the press?

Polyamide chains carry amide groups, and amide groups hold water through hydrogen bonds. As water enters the polymer it acts as a plasticizer: intermolecular forces weaken, the glass transition temperature falls, and the part increases in volume and dimension, in the words of the LANXESS conditioning document. The process is reversible — dry the part and it gives the water back.

This is a different mechanism from drying before moulding. Pre-mould drying limits moisture in the melt so the process stays stable and the resin does not hydrolyse; we covered that step separately. Service moisture arrives after ejection, no matter how well the pellets were dried. But this doesn’t tell the entire picture: crystallinity, fillers and wall thickness all change how fast and how far the part moves.

Two mirrored black moulded housings from a 1+1 family cavity set
Moulded housings like these change state after ejection, not just during moulding.

How much water does each grade take on, and how fast?

The LANXESS document publishes equilibrium water content for six polyamide types under two conditions: storage at 23 °C and 50% relative humidity, and full saturation in water at 23 °C.

PolyamideEquilibrium at 23 °C, 50% RHSaturated in water at 23 °C
PA63.0%10.0%
PA662.8%9.0%
PA464.3%12.0%
PA6102.0%3.8%
PA110.8%1.5%
PA120.8%1.5%
Water content by weight. Source: LANXESS, water absorption and conditioning of Durethan mouldings.

From PA6 to PA12 the equilibrium gap is 3.0% against 0.8%. Tight-tolerance parts start at the low end of that list.

Speed depends on wall thickness. The same document tracks a 2 mm PA6 wall in storage at 23 °C and 50% RH: about 1.5% moisture after 50 hours, about 2.2% after 100 hours, and near equilibrium at 2.8% by 150 hours. Its glass-filled PA6 grade (30% fibre) sits near 1.1% at the same point, because the fibre displaces polymer that would otherwise hold water. DuPont’s datasheet for Zytel 101L gives the companion figures for PA66: 2.7% at 50% RH equilibrium, 8.5% saturation, and 1.2% after 24 hours of immersion.

A thin part therefore does most of its moving within the first week indoors. A thick part keeps creeping toward equilibrium for far longer — the DuPont design manual notes that absorption beyond 4–5% becomes very slow, which is why partial conditioning is standard practice for heavy sections.

What does the water do to stiffness and toughness?

The Zytel 101L datasheet publishes the same grade twice: dry as moulded and conditioned to 50% RH. The two columns answer the stiffness question in one look.

Zytel 101L property (unfilled PA66)Dry as mouldedConditioned, 50% RH
Tensile modulus, ISO 5273100 MPa1200 MPa
Yield stress, ISO 52783 MPa53 MPa
Yield strain, ISO 5274.5%25%
Notched Izod at 23 °C, ASTM D25653 J/m112 J/m
Same grade, two moisture states. Source: DuPont Zytel 101L NC010 datasheet.

Half the stiffness. Twice the impact resistance. One grade of nylon.

The toughness gain is a design resource, not just a side effect. The DuPont design manual allows 6% strain for a snap-fit lug in Zytel 101 at 50% RH against 4% dry, which means a conditioned clip survives assembly moves that would crack a brittle dry one. Strength moves the other way: yield stress falls by about a third. A press-fit or a load-bearing boss sized on dry numbers can creep loose in service.

What should the drawing and the RFQ say?

Three lines of text prevent most of the surprises. First, name the moisture state next to every critical dimension — dry as moulded, or conditioned at 50% RH. Second, state the conditioning procedure when conditioned values are required. Third, name the grade deliberately: PA12 or PA610 when the tolerance is tight, glass-filled PA66 when stiffness must survive humidity.

The DuPont design manual publishes working conditioning procedures, and they are more specific than most buyers expect.

Conditioning parameterPublished value (DuPont design manual)
Target moisture for 50% RH serviceabout 2.5% by weight
Potassium acetate solution boil, 2 mm wallabout 4 hours
Potassium acetate solution boil, 3 mm wallabout 20 hours
Plain boiling waterto about 3% moisture; surface takes up excess
Sections of 3 mm and abovepartial conditioning recommended
Stress relief for service below 70 °Cboiling water, 15 minutes per 3 mm
Conditioning targets and times. Source: DuPont, general design principles for engineering polymers.

Size moves with water. As an illustrative calculation only — using an industry-typical linear swelling figure of 0.25% at 50% RH, which is not a value from the documents cited above — a 50 mm bore grows by about 0.125 mm, more than twice a ±0.05 mm tolerance band. Exact swelling percentages are grade-specific, so the honest defence is the moisture note on the drawing, not an assumed constant.

In our shop, PA parts are measured on the bridge CMM in the dry-as-moulded state unless the drawing says otherwise. When a drawing names a conditioning state, the report matches the state the assembly plant will actually see.

Multi-cavity mould plate with inserts checked on the fitting bench
Tool checking before trials, where cavity-level corrections are still cheap.

Limitations

Test specimens are not your parts. The ISO 62 equilibrium figures come from thin standard plates and the ASTM D570 figures from 3.2 mm discs; a housing with ribs, bosses and variable walls absorbs along different paths and at different speeds. The LANXESS storage-time series is read from published curves, so those values carry an “about” rather than a decimal point of precision.

All quantitative data belongs to DuPont and LANXESS, accessed at the time of writing through their official distributors’ public document mirrors (Distrupol and a DuPont datasheet mirror) because the original portals were unreachable from our network. These are resin-maker laboratory figures for specific grades, not industry-wide guarantees and not our shop measurements. No single accessible document publishes a swelling percentage for PA66, which is why the worked size example above is labelled as an illustration on an assumed input.

What this means for your RFQ

A nylon part is not one size; it is a range, and the drawing picks the point. We help buyers specify the moisture state that decides which size a PA part delivers, and we measure the first articles to match that state on the bridge CMM before the tool is approved.

Send the drawing with a moisture note on it — dry as moulded or conditioned at 50% RH — together with the resin grade and annual volume to info@hongqiangmould.com; the quote lands back within 24 hours (F-004). If a phone call is faster, the WhatsApp button sits on every page.

Specified | Measured | Stable.

Frequently asked questions

How much water does PA66 absorb at room humidity? About 2.7 to 2.8 percent at 23 °C and 50 percent relative humidity, and 8.5 to 9.0 percent when saturated in water. The first figure pair comes from ISO 62 measurements published by DuPont for Zytel 101L and by LANXESS for Durethan PA66. Absorption is reversible and continues until the part matches its surroundings.

Does 2.7 percent moisture mean the part grows 2.7 percent? No. The 2.7 percent figure is water content by weight, not a dimensional change. Water uptake does increase part dimensions, but the linear growth is far smaller than the weight gain, and swelling percentages vary by grade. Treat the published weight figures and any dimensional change as separate properties, and name the moisture state when a size matters.

How long does a nylon part need to reach moisture equilibrium? Wall thickness decides. Published LANXESS data for a 2 mm PA6 wall shows about 1.5 percent moisture after 50 hours and roughly 2.2 percent after 100 hours at 23 °C and 50 percent relative humidity. Thick sections absorb far more slowly, so partial conditioning is recommended once moisture passes 4 to 5 percent.

Can PA66 parts be conditioned before final measurement or assembly? Yes, and resin makers publish procedures. Boiling in a potassium acetate solution caps uptake at 2.5 percent moisture, needing about 4 hours for a 2 mm wall and 20 hours for 3 mm. Plain boiling water reaches roughly 3 percent but can over-saturate the surface. Parts destined for wet service are soaked toward saturation instead.

Jack works on the tooling and molding team at Hongqiang Mould, an injection mould manufacturer and plastic injection molding supplier. The shop runs 11 presses from 80 to 450 T, 5 CNC machining centres and a metrology room with bridge CMM inspection.


Technical Guides

Browse all technical guides →