A Small Shot on a Big Barrel Degrades Before the Mould Opens: Keep the Metering Stroke at 1–3 D (5 Resin Limits, 2 Supplier Rules)

A Small Shot on a Big Barrel Degrades Before the Mould Opens: Keep the Metering Stroke at 1–3 D (5 Resin Limits, 2 Supplier Rules)

← Back to Blog · A Small Shot on a Big Barrel Degrades Before the Mould Opens: Keep the Metering Stroke at 1–3 D (5 Resin Limits, 2 Supplier Rules)

We help buyers keep melt quality stable from the first shot to the last, and the check most quotes skip sits in the barrel. Barrel occupancy decides how long resin waits hot: a 45 g shot fits a 64–150 g cylinder, and polyamide tolerates 4–10 minutes. Clamp tonnage alone tells you neither number.

Barrel occupancy is the share of the cylinder one shot fills. Covestro keeps it between 30 and 70 percent on Makrolon PC datasheets. LANXESS asks for a metering stroke of one to three screw diameters and caps Durethan PA grades at 4 to 10 minutes in the cylinder. Run the same 45 g shot on a 90 g barrel and on a 900 g barrel, and the wait moves from 1.1 minutes to 10.7 minutes at a 32 s cycle. That one ratio separates a fresh melt from a degraded one.

The clamp calculation looks finished, and the press looks booked. Then the first shots come out brown near the gate, and nobody changed a setting.

Machine catalogs pull buyers toward bigger platforms: more tonnage, more shot capacity, more margin. Processing guides from resin makers push the other way. They warn against a machine that is too big for the shot weight, because the melt spends too long hot and molecular weight pays the bill.

The contradiction shows up in quotation requests. Buyers state part weight for the tonnage check, yet the same RFQ rarely carries runner weight or a resin grade — the two numbers the barrel check needs. One side of the press gets a full calculation, the other side gets a guess.

  • What window do datasheets set for shot-to-cylinder size?
  • How long can common engineering resins sit in a hot cylinder?
  • What does the arithmetic change for a mould RFQ?

Based on two supplier documents and one worked example, the barrel check takes about two minutes and catches the failure mode the clamp check cannot see.

Key takeaways

  • Occupancy window: Covestro caps PC shot-to-cylinder size at 30–70 %, so a 45 g shot fits a 64–150 g cylinder.
  • Stroke rule: LANXESS sets the metering stroke at 1–3 × screw diameter; outside it, molecular weight drops or air streaks appear.
  • Resin clock: Durethan PA66 and PA6 grades hold 4–10 min in the cylinder; Pocan PBT grades hold 4–8 min.
  • Worst case: a 45 g shot on a 900 g barrel waits about 10.7 min per 32 s cycle — above the PA ceiling.
  • RFQ fix: state part weight, runner weight and resin grade, so the moulder books the press by barrel as well as by clamp.

Methodology

Two published supplier documents carry every limit quoted here, and one arithmetic example we worked ourselves carries the timings. The first document is the LANXESS processing guide Processing data for the injection molder (LXS-SCP-006EN, 25 pages), which states the metering-stroke rule, the cylinder residence table and the burn-streak remedy for Durethan and Pocan grades. The second is the Covestro product page for Makrolon DQ5142 RE, which lists recommended processing values including shot-to-cylinder size.

Throughout this article, every figure carries its own label. Supplier limits are marked with the source name in the table rows. The worked shots, barrels and cycle times in the third section are a calculated example built for this article — they are not measurements from our moulding floor, and no customer project sits behind them. Brand-specific numbers stay brand-specific: the LANXESS minutes apply to Durethan and Pocan grades, and the Covestro window applies to a Makrolon PC grade. Generic resins can differ, and the Limitations section lists where that matters.

What Is Barrel Occupancy, and Why Do Datasheets Cap It?

Barrel occupancy is the shot weight divided by the rated shot capacity of the cylinder. A 45 g shot inside a 150 g barrel occupies 30 percent. The percentage matters because the melt that is not injected this cycle stays in the hot barrel and waits for the next one.

Covestro writes the window directly into its recommended processing table. The datasheet for Makrolon DQ5142 RE lists shot-to-cylinder size at 30–70 %, next to melt temperature, drying and vent-depth values. LANXESS reaches the same idea from the screw side: the processing guide asks for a metering stroke between 1 and 3 screw diameters, and states that outside this range the mouldings suffer molecular weight reduction from an excessively long residence time, or surface defects from air trapped in the screw.

FieldValueSource
Shot-to-cylinder size (Makrolon PC)30–70 %Covestro DQ5142 RE datasheet
Metering stroke (Durethan, Pocan)1–3 × screw diameter DLANXESS processing guide, §2.3
PA66 melt temperature275–295 °CLANXESS Table 2
PA6 melt temperature260–280 °CLANXESS Table 2
PBT melt temperature250–270 °CLANXESS Table 2

Two suppliers, two units, one message. Match the melt volume to the barrel.

But datasheet windows assume a steady cycle. A shift with stoppages plays by different rules, and the guide says so in its own troubleshooting table.

How Long Can Resin Sit in the Cylinder Before It Degrades?

The LANXESS guide publishes a residence-time table for its engineering grades. The values apply to general-purpose, non-flame-retardant products and serve as a guide, as the document states. Every row lands between 4 and 10 minutes.

Resin (LANXESS grades)Melt temperatureResidence limit
PA66, unreinforced275–295 °C4–10 min
PA66, glass-filled280–300 °C4–10 min
PA6, unreinforced260–280 °C4–10 min
PA6, glass-filled270–290 °C4–10 min
PBT and PBT GF250–270 °C4–8 min

Glass filling changes little here. Heat sensitivity, not stiffness, sets the clock.

The same guide carries a fault table for brown streaks. Its remedy line reads: reduce cycle time, use a smaller plasticating unit. The guide also warns directly against long residence times caused by a machine that is too big for the shot weight. In other words, the supplier names the oversized press as a root cause, not as a safety margin.

What Happens When a 45 g Shot Runs on a 900 g Barrel?

A workable estimate uses the ratio between barrel capacity and shot weight: residence time ≈ (barrel capacity ÷ shot weight) × cycle time. Take a calculated example. A part weighs 38 g, the runner adds 7 g, so the shot is 45 g. The cycle runs at 32 s. Four barrel sizes then give four very different waits.

Barrel capacityShots in barrelOccupancyResidence time at 32 s
90 g2.050 %≈1.1 min
150 g3.030 %≈1.8 min
300 g6.715 %≈3.6 min
900 g20.05 %≈10.7 min

Only the 90 g and 150 g barrels sit inside the Covestro window. The 900 g barrel quadruples the wait.

Ten point seven minutes crosses the 10-minute PA ceiling before anyone touches a temperature setpoint. The burn-streak row in the LANXESS fault table describes exactly this situation, and its fix is not a heater adjustment — it is a smaller plasticating unit. Melt degradation from over-long residence also shows up as black specks and brittle parts, long before a dimension moves.

Yet the ratio alone misses one thing. A long wait harms heat-sensitive resins first; PP and PE shrug off waits that would ruin PA66. The example barrel sizes are illustrative, and real machines carry several screw-and-barrel combinations per clamp tonnage. The ratio is the check, not the press badge.

Upper and lower housing covers moulded in light grey resin
Two housing covers like these can weigh less than the runner that feeds them.

Which Press Details Belong in Your RFQ?

Across our eleven presses (80–450 T), one mould often clears the clamp check on several machines. The barrel decides which machine takes the job. Three inputs make that decision clean on both sides.

  • Shot weight: part plus runner, in grams — the runner share is real material with a real clock.
  • Resin grade: the name on the datasheet, not just the polymer family.
  • Expected cycle time: even a rough range turns the occupancy ratio into minutes.

Runner weight deserves its own line, because small parts carry proportionally heavy feed systems; our earlier piece on cold runners shows how much resin a channel adds on a 12 g part. Our clamp-side walkthrough covers the other half of the press decision, and the two checks together take one page in an RFQ.

One caveat sits beyond the table. A moulder can also downsize the shot with a spacer bushing or a smaller injection unit on the same clamp frame. That is a conversation worth having before the steel order, not after the first brown streak.

Limitations

Datasheet windows describe steady production, not a shift with stoppages. The LANXESS guide tells processors to drop the screw forward, cut the barrel temperature or switch off heating during long interruptions, and to purge with fresh granules afterwards. Every estimate in this article assumes the melt keeps moving; a machine park delay resets the clock in a harsher way than any barrel size does.

Every limit quoted here comes from supplier documents, not from trials run on our floor. The residence minutes belong to Durethan PA and Pocan PBT grades, and the 30–70 % window belongs to a Makrolon PC grade; flame-retardant grades carry their own restrictions, as the guide itself notes. This article cites the LANXESS guide through a public web archive copy because the original download was not reachable at writing time. Other suppliers publish similar windows with slightly different edges, and the specific datasheet for your grade always wins over a general table.

What This Means for Your Next Mould Project

We help procurement teams turn a drawing into a press booking that survives both checks: clamp tonnage from the projected area, and barrel fit from shot weight against the occupancy window. Send the 3D file, the resin grade and the runner plan to info@hongqiangmould.com or message +86 199 6437 6528 on WhatsApp, and the quotation lands within 24 hours. From first article to series production, one shop carries both checks — the clamp side and the barrel side.

Stable | Uniform | On Cycle

Frequently asked questions

What is barrel occupancy in injection moulding? Barrel occupancy is the shot weight divided by the rated capacity of the cylinder, written as a percentage. Covestro lists an acceptable window of 30 to 70 percent on Makrolon PC datasheets. Below the window the resin waits too long in the barrel, and above it the screw runs short of melt reserve.

How do you estimate residence time before the first shot? Divide the barrel capacity by the shot weight, then multiply by the cycle time. A 900 g barrel running a 45 g shot on a 32 s cycle holds 20 shots, so the melt waits roughly 10.7 minutes. Compare that figure with the resin limit before you book the press.

Which resins degrade fastest in a hot barrel? Polyamide and PBT sit on the short end. LANXESS caps Durethan PA66 and PA6 grades at 4 to 10 minutes in the cylinder, and Pocan PBT grades at 4 to 8 minutes. Long stays push molecular weight down and show up as brown streaks or brittle parts.

Does a bigger press always make part quality worse? The clamp force itself does no harm. The risk sits in the injection unit, because an oversized barrel stretches residence time beyond the resin limit. Pick the smallest press that passes the clamp check and the occupancy window at the same time, and the melt stays fresh.

Jack works on the tooling and molding team at Hongqiang Mould, an injection mould manufacturer and plastic injection molding supplier. The shop runs 11 presses from 80 to 450 T, 5 CNC machining centres and a metrology room with bridge CMM inspection.


Technical Guides

Browse all technical guides →